Technical8 min read

AS 3700 and Older Masonry: What Engineers Check Before You Cut an Opening or Remove a Wall

TR
TRSC Engineering

Loadbearing masonry is one of the more deceptive structural materials in older Queensland buildings. It looks solid. It has stood for decades. And because it has stood, owners and builders often assume it will accommodate whatever comes next: a wider doorway, a removed wall, a new storey above. That assumption has caused collapses.

AS 3700:2018, *Masonry Structures*, sets out how masonry is designed today. AS 4773, *Masonry in Small Buildings*, covers residential and small commercial work. But Queensland has a substantial stock of brick and block construction from the 1890s through to the 1980s that predates both standards entirely. Those buildings were designed under different codes, different material specifications, and sometimes no formal code at all. Before any alteration, an engineer needs to understand what is actually there, not what a standard assumes.

What the Wall Is Made Of

The first question is construction type. Older Queensland masonry falls into several categories, and they behave very differently under load.

Solid brick walls are the most common in pre-1960s construction. A 230 mm solid wall carries load through its full thickness. A 350 mm or 450 mm wall, common in older commercial buildings, has real compressive capacity but almost no lateral resistance without returns or cross-walls.

Cavity walls became standard from roughly the 1950s onward. Two leaves of brickwork are separated by a 50 mm air gap and tied together with metal wall ties. The outer leaf handles weathering; the inner leaf carries floor and roof loads. The cavity construction means the two leaves must act together for stability, which is only possible if the ties are intact.

Reinforced concrete block walls appeared widely from the 1960s. Hollow blocks with vertical reinforcement grouted in place can carry significant load, but the condition of the grout and the continuity of the reinforcement are not visible from the surface.

Determining which type you have requires more than looking at the face of the wall. Drilling a small inspection hole, using a borescope, or reviewing original drawings (where they exist) is often necessary. Wall thickness measured at a window or door reveal gives a starting point, but it does not distinguish a solid wall from a cavity wall of similar overall thickness.

The Load Path Above

Before touching a loadbearing wall, an engineer traces every load that passes through it. Timber floor joists bearing onto an internal brick wall, a concrete slab transferring load to a perimeter wall, roof trusses sitting on a top plate that sits on brick: each of these creates a load path that must be maintained or redirected during and after the alteration.

In Queensland's older Queenslander-style construction, the situation is often complicated by subfloor framing that has been modified over decades, with loads redistributed in ways that were never documented. A wall that appears non-loadbearing may be carrying point loads from a beam above, or may be providing lateral restraint to a long timber wall plate.

Roof loads deserve particular attention. Hip roofs, common in Queensland, spread load to perimeter walls along their full length. Removing a section of wall without understanding how the roof structure bears can introduce concentrated loads at the remaining piers that the masonry was never designed to carry.

Mortar Condition and Compressive Strength

Masonry derives its compressive strength from the combined behaviour of units and mortar. In older construction, mortar was typically lime-based: softer, more flexible, and more permeable than modern cement mortars. Lime mortar weathers and erodes over time, particularly in exposed locations or where water has been entering through failed flashings or cracked render.

Visual inspection of mortar joints gives a rough indication of condition. Joints that are recessed more than 5 mm, friable when probed with a key, or showing powdering and loss of cohesion are a concern. But visual inspection cannot quantify strength. Where the assessment depends on mortar capacity, in-situ testing is warranted. The most practical method for existing masonry is scratch hardness testing combined with laboratory analysis of mortar samples extracted by coring. This allows an estimate of compressive strength that can be compared against AS 3700 assumptions.

For walls that will carry new or redirected loads after an alteration, mortar strength is not an academic question. A wall with mortar compressive strength of 1 MPa behaves very differently from one at 5 MPa, and AS 3700 capacity calculations are sensitive to this input.

Lintels and Arching Action

Every existing opening in a masonry wall has either a lintel or relies on arching action, or both. Understanding which is doing the work matters when you are proposing to enlarge an opening or add load above it.

Older lintels in Queensland buildings are commonly timber, steel angle, or unreinforced brick soldier courses. Timber lintels decay, particularly where moisture has entered. Steel angle lintels corrode, and the expansion of corroding steel can crack the brickwork above. Brick soldier lintels have limited span capacity and are vulnerable to differential settlement.

Arching action is the tendency of masonry above an opening to redistribute load around the opening through a natural arch, provided there is sufficient masonry above and adequate abutments on either side. AS 3700 recognises arching action, and it is a real phenomenon in older walls with sufficient height above the opening. But it depends on the masonry being intact and the abutments being capable of resisting the horizontal thrust the arch generates. Where cracking has disrupted the arch geometry, or where an adjacent opening reduces the available abutment, arching action cannot be assumed.

When an existing opening is to be widened, the engineer must assess whether the existing lintel can span the new width, whether arching action remains viable, and what new lintel section is required. This is not a rule-of-thumb exercise in older masonry.

Wall Ties in Cavity Construction

Cavity wall ties are the connection between the two leaves. Without them, the outer leaf acts as an unrestrained panel with very limited capacity to resist wind loads or its own self-weight over height. In Queensland, where cyclone-region wind classifications apply to much of the coast and wind loads are a design driver even in Brisbane, tie condition is not a minor detail.

Ties in pre-1980s construction were typically galvanised mild steel. Galvanising standards were lower than current requirements, and in coastal or humid environments, corrosion is common. Corroded ties lose section and eventually lose load transfer capacity entirely. In advanced cases, the expanding corrosion product causes horizontal cracking or spalling at the mortar bed level.

Tie condition cannot be assessed from the wall surface. Borescope inspection through drilled holes, or selective removal of bricks, is required. Where ties are found to be corroded, the outer leaf must be treated as effectively unrestrained for structural purposes until remediation is completed.

Reading Distress Before You Alter Anything

Existing cracking and deformation in a masonry wall is information. It tells you what the wall has already experienced and, in some cases, what it is still experiencing.

Stepped cracking following mortar joints in a staircase pattern is the classic sign of differential settlement. The crack path follows the weakest plane, which in older lime mortar construction is usually the joint rather than the unit. Stepped cracking at corners or adjacent to openings indicates that the foundation or subsoil has moved. Before any alteration, the cause of that movement needs to be understood. Altering a wall that is still settling can accelerate the distress.

Vertical cracking at the junction between a masonry wall and a return, or at a change in wall thickness, often indicates thermal or moisture movement rather than structural overload. But the same crack pattern can also indicate loss of connection between perpendicular walls.

Bulging in a cavity wall outer leaf is a serious finding. It indicates that the ties have failed or the outer leaf has become detached from the inner leaf. A bulging outer leaf is unstable and can fall without further warning. Any alteration work in the vicinity of a bulging wall requires the outer leaf to be made safe before other work proceeds.

Lintel corrosion cracking appears as horizontal cracking at the level of a steel lintel, often with rust staining. The lintel is expanding as it corrodes, and the masonry above is being pushed apart. The lintel's remaining structural capacity is likely reduced.

Each of these distress types changes the assessment. A wall with active settlement, failed ties, or a corroding lintel is not a wall that can simply be opened up and spanned with a new beam. The distress must be addressed as part of the alteration scope.

Temporary Support During Works

When a loadbearing wall is to be opened or removed, the loads it carries must be transferred to temporary works before any masonry is cut. This means acrow props, strongbacks, and needle beams sized for the actual loads, not estimated. The temporary support must be in place and verified before the first brick is removed.

In older buildings, the floor structure bearing onto the wall may itself be in poor condition. Timber floor joists affected by decay or borer damage may not be capable of transferring loads to temporary props without local reinforcement. The temporary works design must account for this.

Queensland's building legislation requires that structural alterations to loadbearing elements be designed by a Registered Professional Engineer of Queensland (RPEQ) and certified accordingly. The temporary works are part of that scope.

What Testing Actually Tells You

For older masonry where the construction history is uncertain, two tests change the quality of the assessment substantially: mortar strength testing and wall tie inspection.

Mortar samples extracted by coring can be tested in a NATA-accredited laboratory for compressive strength and composition. The composition result tells you whether the mortar is lime-based, cement-lime, or cement-rich, which informs both the strength estimate and the likely behaviour under load redistribution.

Wall tie inspection by borescope, combined with a tie count from the original construction records where available, tells you whether the cavity wall can be treated as a composite section or must be assessed as two independent leaves.

Without this data, an engineer assessing an older masonry wall for alteration is working with assumptions. Those assumptions must be conservative, which means the remediation or alteration design will also be conservative, and the cost will reflect that. Testing narrows the uncertainty and often reduces the scope of intervention required.

The Assessment Before the Alteration

The sequence matters. An engineer assessing an older masonry wall for a proposed alteration needs to establish wall construction type, load path from above, mortar condition, lintel condition and capacity, tie condition in cavity walls, and existing distress before any design work begins. Where the evidence is insufficient, targeted testing fills the gaps.

This is not a process that can be compressed into a site visit and a rule-of-thumb calculation. Older masonry has a history, and that history is embedded in the wall. Reading it correctly is what separates a safe alteration from one that creates problems the builder discovers mid-construction.

If you are planning an opening, a wall removal, or an added storey in an older Queensland masonry building, TRSC provides structural assessments that work from measured evidence rather than assumptions. More information is available at https://trsc.au.

Back to blog

Need structural engineering expertise?

TRSC specialises in complex existing assets, heritage buildings, aging infrastructure, and post-disaster assessment.

Book a Consultation